KONPONÈ CHIMIK:
ALLOY (poids%) | C | Mn | Si | Cr | Fe | Al | Cu | P | S |
RÈG GB/T | 2.00 | 2.50 | 4.00 | 45-60 | Marge | 1.00 | 2.50 | - | 0.03 |
RÈG AWS | 2.00 | 2.50 | 4.00 | 45-60 | Marge | 1.00 | 2.50 | - | 0.03 |
EGZANP VALÈ | 0.59 | 0.26 | 0.93 | 55.1 | 42.8 | 0.18 | 0.03 | 0.023 | 0.005 |
PWOPRIYETE MEKANIK:
PWOPRIYETE | FÒS RENDE (MPa) | FÒS ekstansyon (MPa) | VALÈ IMAPACT J/℃ | ELONGATION (%) | ||||
RÈG GB/T | - | - | - | - | ||||
RÈG AWS | - | - | - | - | ||||
EGZANP VALÈ | - | - | - | - |
PARAMÈT SOUDE REKÒMANDE:
DYAMET SPECIFICATIONS (mm) | 2.6 * 300 | 3.2 * 350 | 4.0 * 350 | 5.0 * 350 | ||||
ELEKTRIS(Amp) | H/W | 60-80 | 80-120 | 120-150 | 130-180 |
Elektwòd la se fil nwayo nikèl, fò elektwòd fè jete grafitize.
Lè soude, soude a pa ka prechofe.
Li gen karakteristik segondè fòs, bon plastisit, ekselan rezistans fann ak bon fizyon ak metal debaz.
-
Lachin Syans & Teknoloji co, LTD. 20 milyon tòn/ane raffinage ak pwojè entegrasyon chimik
-
Materyèl soude pou resipyan
Shaanxi Pucheng -50 ℃ pwopan pwojè tank esferik
KONPONÈ CHIMIK:
ALLOY (poids%) | C | Mn | Si | Cr | Fe | Al | Cu | P | S |
RÈG GB/T | 2.00 | 2.50 | 4.00 | 45-60 | Marge | 1.00 | 2.50 | - | 0.03 |
RÈG AWS | 2.00 | 2.50 | 4.00 | 45-60 | Marge | 1.00 | 2.50 | - | 0.03 |
EGZANP VALÈ | 0.59 | 0.26 | 0.93 | 55.1 | 42.8 | 0.18 | 0.03 | 0.023 | 0.005 |
PWOPRIYETE MEKANIK:
PWOPRIYETE | FÒS RENDE (MPa) | FÒS ekstansyon (MPa) | VALÈ IMAPACT J/℃ | ELONGATION (%) | ||||
RÈG GB/T | - | - | - | - | ||||
RÈG AWS | - | - | - | - | ||||
EGZANP VALÈ | - | - | - | - |
PARAMÈT SOUDE REKÒMANDE:
DYAMET SPECIFICATIONS (mm) | 2.6 * 300 | 3.2 * 350 | 4.0 * 350 | 5.0 * 350 | ||||
ELEKTRIS(Amp) | H/W | 60-80 | 80-120 | 120-150 | 130-180 |